	To remove Technovit 7200 and re-embed in methyl methacrylate(mma):
Remove all excess solid Technovit and place in liquid Technovit 7200 with
stirring and light inhibiting cover.  Check daily and remove outside gummy
areas.  Depending on the size of the specimen, this can take some time (up
to 2 weeks for large specimens).  Place in inhibited, liquid methyl
methacrylate and stir for  a couple of days.  Place in final mma and allow
to polymerize.
	Linda
*********************************